材料materjal |
厚度 paksud (mm) |
速度Kiirus (m/min) |
功率 Võimsus (W) |
气体 Gaas |
气压 Surve (baar) |
喷嘴Düüsid (mm) |
焦点 位置 Keskendu Punkt (mm) |
切割高度 Lõikamine Kõrgus (mm) |
备注 Rema rk |
碳钢 |
1 |
60-80 |
12000 |
N2/ |
8 |
2.0 |
0 |
0.5 |
1 |
Süsinik Teras |
2 |
45-50 |
Õhk |
8 |
3.0 |
-0.5 |
0.5 |
||
3 |
32-38 |
8 |
3.0 |
-1 |
0.5 |
||||
4 |
23-28 |
8 |
3.0 |
-1 |
0.5 |
||||
5 |
20-23 |
8 |
4.0 |
-2 |
0.5 |
||||
6 |
16-20 |
8 |
4.0 |
-2 |
0.5 |
||||
8 |
10-13 |
8 |
5.0 |
-3 |
0.5 |
||||
10 |
5,5-7,5 |
10 |
5.0 |
-3 |
0.5 |
||||
12 |
4,0-5,5 |
16 |
5.0 |
-3 |
0.5 |
||||
8 |
2,3-2,5 |
4000 |
O2 |
0.6 |
1.2 |
+10 |
0.6 |
||
10 |
2,0-2,2 |
6000 |
0.6 |
1.2 |
+11 |
0.6 |
|||
12 |
1,8-2,0 |
6000 |
0.6 |
1.2 |
+12 |
0.6 |
|||
14 |
1,6-1,8 |
8000 |
0.6 |
1.4 |
+12 |
0.6 |
|||
16 |
1,5-1,7 |
8000 |
0.5 |
单 1.4 Üksik |
+13 |
0.5 |
|||
18 |
1,6-1,7 |
10000 |
0.5 |
单 1,5 vallaline |
+14 |
0.5 |
|||
20 |
1,4-1,6 |
12000 |
0.5 |
单 1,5 vallaline |
+15 |
0.5 |
|||
22 |
1,3-1,5 |
12000 |
0.5 |
单 1,5 vallaline |
+15 |
0.5 |
|||
25 |
1,0-1,2 |
12000 |
0.55 |
单 1,5 vallaline |
+15 |
0.5 |
|||
碳钢 Süsinik Teras |
30 |
0,8-1,0 |
12000 |
O2 |
0.7 |
单 1.7 Üksik |
+16 |
0.5 |
|
35 |
0,5-0,7 |
12000 |
1.5 |
单 1.7 Üksik |
+17 |
0.5 |
|||
40 |
0,3-0,4 |
12000 |
1.2 |
单 1.7 Vallaline |
+17 |
0.5 |
|||
不锈钢 |
1 |
60-80 |
12000 |
N2 |
8 |
2.0 |
0 |
0.5 |
Roostematerjalid s Teras |
2 |
60-70 |
8 |
3.0 |
-0.5 |
0.5 |
|||
3 |
50-60 |
8 |
3.0 |
-0.5 |
0.5 |
||||
4 |
35-43 |
8 |
3.0 |
-1 |
0.5 |
||||
5 |
20-25 |
8 |
4.0 |
-1.5 |
0.5 |
||||
6 |
18-22 |
8 |
4.0 |
-2 |
0.5 |
||||
8 |
15-17 |
8 |
5.0 |
-3 |
0.5 |
||||
10 |
7,0-8,0 |
8 |
5.0 |
-3 |
0.5 |
||||
12 |
6,0-7,0 |
18 |
5.0 |
-3 |
0.5 |
||||
14 |
4,0-5,0 |
18 |
5.0 |
-5 |
0.5 |
||||
16 |
2,5-3,0 |
20 |
5.0 |
-6 |
0.5 |
||||
18 |
1,6-2,0 |
20 |
5.0 |
-10 |
0.5 |
||||
20 |
1,4-1,5 |
20 |
5.0 |
-11 |
0.3 |
||||
22 |
1,2-1,4 |
20 |
5.0 |
-12 |
0.5 |
||||
25 |
0,8-1,2 |
20 |
6.0 |
-13 |
0.5 |
||||
30 |
0,3-0,4 |
25 |
5.0 |
7 |
0.5 |
||||
35 |
0,2-0,3 |
25 |
5.0 |
7 |
0.5 |
||||
40 |
0,1-0,15 |
25 |
5.0 |
7 |
0.5 |
||||
铝合金Alumiinium um Sulam |
1 |
60-80 |
12000 |
N2 |
8 |
2.0 |
0 |
0.5 |
|
2 |
60-70 |
8 |
3.5 |
-1 |
0.5 |
||||
3 |
40-50 |
10 |
3.0 |
-1 |
0.5 |
||||
4 |
30-35 |
12 |
3.0 |
-1 |
0.5 |
||||
5 |
25-30 |
13 |
3.5 |
-1.5 |
0.5 |
||||
6 |
20-25 |
16 |
4.0 |
-2.5 |
0.5 |
||||
8 |
10-12 |
16 |
4.0 |
-2 |
0.3 |
||||
10 |
5,0-6,0 |
16 |
4.0 |
-3 |
0.5 |
||||
12 |
3,0-4,0 |
16 |
5.0 |
-2 |
0.3 |
||||
14 |
2,0-2,5 |
16 |
5.0 |
-4 |
0.3 |
||||
16 |
1,6-2,0 |
16 |
5.0 |
-4 |
0.3 |
||||
18 |
1,4-1,6 |
20 |
5.0 |
-5 |
0.5 |
||||
20 |
1,2-1,4 |
20 |
5.0 |
-5 |
0.5 |
||||
25 |
0,8-1,0 |
20 |
5.0 |
-6 |
0.5 |
||||
30 |
0,4-0,6 |
20 |
5.0 |
-6 |
0.3 |
||||
35 |
0,2-0,3 |
20 |
5.0 |
+7 |
0.3 |
||||
黄铜 Messing |
1 |
60-80 |
12000 |
N2 |
8 |
3.0 |
-1 |
0.5 |
|
2 |
50-60 |
8 |
3.0 |
-1 |
0.5 |
||||
3 |
40-50 |
8 |
3.0 |
-1 |
0.5 |
||||
4 |
30-35 |
10 |
3.0 |
-1.5 |
0.5 |
||||
5 |
25-30 |
10 |
4.0 |
-2 |
0.5 |
||||
6 |
20-25 |
10 |
4.0 |
-3 |
0.5 |
||||
8 |
10-13 |
10 |
5.0 |
-3 |
0.5 |
||||
10 |
5,0-6,0 |
12 |
5.0 |
-3.5 |
0.5 |
||||
12 |
4,0-5,0 |
13 |
5.0 |
-4 |
0.5 |
||||
14 |
2,0-3,0 |
14 |
5.0 |
-5 |
0 |
||||
16 |
1,5-2,0 |
18 |
5.0 |
-6 |
0.5 |
||||
紫铜 Vask |
1 |
50-60 |
12000 |
O2 |
8 |
3.0 |
0 |
0.5 |
3 |
2 |
40-50 |
8 |
3.0 |
0 |
0.5 |
||||
3 |
30-36 |
10 |
3.0 |
-1 |
0.5 |
||||
4 |
20-24 |
12 |
3.5 |
-2 |
0.5 |
||||
5 |
15-18 |
13 |
4.5 |
-2 |
0.5 |
||||
6 |
9,0-11 |
14 |
5.0 |
-3 |
0.5 |
||||
8 |
6,0-7,0 |
14 |
5.0 |
-3 |
0.5 |
||||
10 |
3,0-3,5 |
16 |
5.0 |
-4 |
0.5 |
||||
12 |
2,0-2,5 |
16 |
5.0 |
-4 |
0.5 |
备注 1:碳钢 1-6mm推荐使用空气或氮气切割,切割速度比用氧气的更快,会有轻微挂渳懨。 2:根据现场气体纯度、板材质量等方面的不同,调试所使用的功率以及调试的速度也会有所不同.备注. 3:紫铜需
使用高压氧气切割,使用其他气体切割可能会有损坏激光器得风险。备注:表中红标参数为打样参数,在实际加工中受各类因素影响较大,仅适合小批量生产,不推荐大批量生产加工,建议使用更高功率激光器.
Märkus: Süsinikteras ja roostevaba teras, nagu õhk, lämmastikuga lõikamine, tõhusus ja stabiilsus paranevad, suurendades paksust, kuid kalduvad ka rippuva räbu nähtusele, ülaltoodud andmeparameetrid tegelikul massilõikamisel, tööpingil, süsteemil, lõikepeal, õhurõhul, materjalidel ja muudel teguritel, võib esineda mitmesuguseid muudatusi, tabelis olevad andmed võivad mõjutada mitmesuguseid töötlemisvõimalusi, tabelis olevad andmed, punase märgi parameetrid sobivad ainult tõestuseks. partii tootmine. Masstootmine ei ole soovitatav. Soovitatav on kasutada suurema võimsusega lasereid. Vask tuleb lõigata kõrgsurve hapnikuga, õhk või lämmastik võivad laserit kergesti kahjustada.
11,2 单模块 MFSC-12000W 纤芯 50 μm 穿孔参考 ühe mooduliga MFSC-12000W kiudsüdamiku 50 μm perforatsiooni võrdlus
11.2.2创鑫MFSC-12000W 25mm碳钢穿孔参数(仅供参考)MAX MFSC-12000W 25mm süsinikterasest perforatsiooniparameetrid (ainult viitamiseks)
阶段lava |
功率 Võimsus (W) |
占空比kohustus suhe (%) |
频率Freque ncy (Hz) |
喷嘴高度Düüsid Kõrgus (mm) |
气压 Õhk Pressu re (baar) |
焦点 Keskendu Punkt (mm) |
穿孔时间Aperture Aeg (ms) |
停光吹气 Peatus puhub (ms) |
高位 |
12000 |
45 |
100 |
20 |
0.8 |
-4 |
200 |
|
Kõrge pos tsioon |
||||||||
中位 Keskmine lk positsioon |
12000 |
45 |
100 |
12 |
0.8 |
-6 |
1500 |
|
低位 Madala positsiooniga mine |
12000 |
45 |
100 |
8 |
0.7 |
-8 |
1000 |
11.2.2 创鑫 MFSC-12000W 20mm 不锈钢氮气穿孔参数(仅供参考)
阶段lava |
功率 Võimsus (W) |
占空比kohustus suhe (%) |
频率Freque ncy (Hz) |
喷嘴高度Düüsid Kõrgus (mm) |
气压 Õhk Pressu re (baar) |
焦点 Keskendu Punkt (mm) |
穿孔时间Aperture Aeg (ms) |
停光吹气 Peatus puhub (ms) |
高位 Kõrge pos tsioon |
12000 |
55 |
3000 |
20 |
10 |
-8 |
200 |
|
中位 Keskmine lk positsioon |
12000 |
45 |
2500 |
12 |
10 |
-12 |
1500 |
|
低位 Madala positsiooniga mine |
12000 |
45 |
2500 |
8 |
10 |
-16 |
500 |
Seotud tooted
sisu on tühi!
Seotud ajaveebid